Afternoon guys, I hope you're all well

I apologise in advance as this is going to be a pic heavy and long post lol
Got the week off as had to use up some hol. Although only today could I get round to welding as was with the mrs yesterday and Monday. anyways I digress lol
Firstly, I used the ''pee shooter'' that recently arrived...... was indoors on max ''6'' on the regulator and only got 5LPM. this is clearly the reason why my welds look not that great lol is there a known problem with this Clarke welder and its gas distribution? im sure ive heard someone mention this. kev perhaps?

So anyways, today's exercise was to weld some beads on all different thicknesses of steel and actually get the settings written down so that I can simply refer to my notebook for the correct setting / wire speed. Then once that was all noted down I would try the methods we've discussed to get this good penetration on some butt welds.
Ok, so some 4mm. I only laid a couple of beads cos quite honestly I'm not convinced this welder will join 4mm that easily and in honesty I probably wont be focusing on this sort of thickness. anyways I noted the best setting for a nice sizzle was MAX 2 - W/S - 6.5
[IMG]
Some 3mm beads... setting MAX 2 - W/S 6
[IMG]
Some 2mm beads.... setting MAX 2 - W/S 5
[IMG]
And some 1.5mm beads... setting MAX 2 - W/S 5
[IMG]
The interesting thing about these is that I found I could weld the 1.5mm on the max heat setting. I did notice that the metal easily distorted though so I'm thinking that I either dial the heat down or when welding I will attack it in short bursts so as not to distort it.
As per the videos posted by norlander i think, I also found that doing loops with the puddle / pool got that classic weld look lol so will do that from now on too

So as of now I'm totally comfortable laying beads on top of steel. check point 1 made lol

So miving on to some butt welds...
3.5mm...with a root gap of about 1.5mm....
[IMG]
you can see in the pic that the inner most weld is a bit fat. I noticed this and then did the smaller weld closest to the bottom of the pic. the reason it was fat initially was cos I was experimenting with travel speed:the fat one was very slow.
as you can see even with a root gap the penetration is still showing the two joins...
[IMG]
A 2mm butt weld....
[IMG]
really not pretty and I think I really suffered from gas distribution issues here. but hey ho.
This 2mm join was a tad better...
[IMG]
my camera died so couldn't get any other shots of penetetration but theyre all the same and all are showing the gap still. where to go from here?
is it something I should be worrying about bearing in mind I beat the living crap out of it and the first thing to bend was the centre of the steel and not my weld lol....
[IMG]
around all the butt welds im getting a real nice ''heat leach'' but as said no weld filtering through the gap.
anyway to end on a high. I did a 1.5mm lap weld and its prob my best looking weld so far....
[IMG]
[IMG]
What do you think guys? and any help with the gap still showing issue would be awesome